Two alloy names come up constantly in Chinese screen supply and almost never in Western material handbooks: 809C and 202B. They are not exotic in the corrosion sense — they are the opposite. They exist because nickel is expensive, and because manganese plus nitrogen can replace most of it while making the steel harder wearing than the grade it replaces.
What the two grades actually are
| Designation | 202B | 809C (E200) |
|---|---|---|
| Chinese standard | 12Cr18Mn8Ni5N | 10Cr21Mn16NiN |
| UNS | S35450 | no direct UNS equivalent |
| Nearest Western grade | ASTM 202 / S20200, EN 1.4373 | no close equivalent |
| Carbon | 0.10–0.15 % | ~0.10 % |
| Manganese | 8–10 % | ~17 % |
| Chromium | 17–19 % | ~20.5 % |
| Nickel | 4.5–6 % | ~1.5 % |
| Nitrogen | 0.20–0.30 % | ~0.63 % |
| Structure | austenitic | austenitic, fully non-magnetic |
202B is a standard 200-series grade: a recognised, documented alloy with published equivalents. 809C is a step further out — 17 % manganese and 0.6 % nitrogen is not a composition any Western mill lists, and it exists as a Chinese screen-industry grade rather than as a book alloy. That has a practical consequence for a buyer: 202B can be cross-checked against a mill certificate and a published specification, and 809C cannot. Ask for a full chemical analysis per heat, not a grade name.
What manganese is doing there
Manganese is an austenite stabiliser. It holds the face-centred cubic structure that gives stainless its toughness and ductility, and it does the job at a fraction of the cost of nickel. Push it to 17 % and you can drop nickel to 1.5 % and still have a fully austenitic, fully non-magnetic steel.
The cost of that substitution is corrosion resistance. Nickel does two things in a stainless steel: it stabilises austenite, and it helps the passive film re-form after it is damaged. At 1.5 % there is very little of the second effect. Add manganese sulphide inclusions, which are efficient pitting initiation sites, and you have an alloy that will pit in chloride water where 304 survives.
What nitrogen is doing there
Nitrogen is the reason these grades are worth using at all. In solid solution it strengthens the austenite — roughly 30–50 MPa of yield strength per 0.1 % — and it raises the work-hardening rate sharply.
That second effect is the wear mechanism. These alloys do not start out exceptionally hard. They get hard where they are abraded: the surface layer deforms, dislocations multiply, and the hardness climbs well above the bulk value. A screen wire in an ore slurry work-hardens at the slot edges as it wears, so the rate of wear slows instead of accelerating. This is why a 1.5 % nickel alloy can outlast 304 three to one in the same duty, which looks impossible if you only compare starting hardness.
Non-magnetic, and why 304 is not
Austenitic grades are nominally non-magnetic, but 304 stops being non-magnetic once it is cold worked. Drawing a V-profile introduces deformation-induced martensite, and a drawn 304 wire will pull a magnet. In magnetic separation, in feed lines ahead of a tramp-iron magnet, or anywhere the screen sits in a magnetic field, that matters.
202B and 809C are more resistant to this because manganese and nitrogen both raise the stacking fault energy and suppress the martensite transformation. For a screen in a magnetite circuit or under a suspended magnet, a high-manganese grade is not just cheaper — it is the only one that behaves.
The limit: welding
This is the part that decides how these grades can be used, and it is where most of the failures come from.
High nitrogen plus high manganese is a difficult weld. Nitrogen comes out of solution in the weld pool and forms porosity; the weld metal is hot-short and cracks under restraint; the as-welded zone loses corrosion resistance relative to the parent metal. On a wedge wire panel with hundreds of automatic spot welds, that combination is a problem, not a detail.
Three ways to work within the limit:
- Reduce weld density. Fewer, larger welds instead of a dense automated pattern — more reliance on bar spacing and wire tension, less on the weld.
- Mechanical fixing. Dovetail or wedge-lock bars that hold the wire profile mechanically, so the screen has few or no welds in the wetted area.
- Woven or punched construction. Where the duty allows, a woven mesh or a punched plate in 809C avoids the welding question entirely.
What that means in practice: these grades are at their best in woven screen, punched plate, sieve baskets and mechanically fixed decks — and they need care in a fully welded cylindrical wedge wire screen. If a supplier quotes a densely welded 809C screen without commenting on the weld procedure, ask what filler and what porosity check they use. The answer tells you whether they have done it before.
Where they belong
Coal preparation and washing plants, ore sizing and dewatering decks, sinter and coke screening, trommel panels, and any abrasive duty where the water is fresh and non-saline. Dry or damp, not acidic, not chloride-bearing.
Where they do not belong: seawater, brine, any acid, any chloride above a few hundred ppm, or food and pharmaceutical contact. Those are 316L, duplex or C276 duty — see duplex wedge wire for the chloride line and C276 for acid.
The comparison across all seven alloys, including the cost-per-wear-life arithmetic, is in abrasion or corrosion first. Both grades are available as V-profile wire and as support bars, and they should be ordered as a matched set. Send the duty, the water chemistry and the solids — if 809C is right, the quotation will say so.
More from ERQI
-
Technical
Wedge Wire Alloy Selection: Abrasion or Corrosion First? | ERQI WIRE
Seven alloys get quoted for wedge wire screens and they are not on one scale. Two questions decide almost every case: is there chloride, and is the duty abrasive. A working decision tree with the numbers behind it.
-
Technical
Wedge Wire, Profile Wire, Shaped Wire: How the Three Names Relate | ERQI WIRE
Three names get used for the same drawn section depending on which industry is buying it. What each name actually means, why buyers pick different words, and how to write an enquiry that works in all three.
-
Business
Small-Batch Custom Shaped Wire: When It Pays | ERQI WIRE
A small batch of custom shaped wire carries the same tooling as a big one. When the arithmetic still works: machined-part replacement, downtime cost, design validation - and when it does not.
Ready to start your project?
Send us your drawing or sample — we reply within 24 hours on working days.